20 ml zirconium oxide (ZrO2) bowl with 20g of 3 mm balls (ZrO2).
Feed quantity:
< 100mg
Feed Size:
< 500 µm
Additive:
+2ml H2O + 3ml Ethanol
Grinding time:
60 min*1
Final fineness:
d50 < 650 nm*2
Comments:
*1: Because of the small amount of sample you will find a lot of abrasion on the grinding set. Grinding steps: 10min grinding + 15min pause (x 6 repetitions).
*2: see the particle size analysis with our Laser-Partikel-Sizer ANALYSETTE 22 -NanoTec on separate page (Meas.-nr. 6709).