M090090 | |
45x20mm | |
< 30µm |
Planetary Mono Mill PULVERISETTE 6 classic line650 U/min |
||
Equipment: |
250 ml zirconiumoxide bowl with 15x20 mm balls (ZrO2) |
|
|
6 glasses | |
|
15 mm*1 | |
|
- | |
|
5 min*2 | |
|
100% < 100 µm d50 <7,4 µm*3 | |
|
*1: We precrushed the glasses with a hammer in a plastic bag to a fineness of 15mm. |
|
Download: | 090090_Glas_P6_ZrO2_2min_01.pdf | |
090090_Glas_P6_ZrO2_5min_01.pdf |
Planetary Mono Mill PULVERISETTE 6 classic line650 rpm |
||
Equipment: |
250 ml zirconiumoxide bowl with 15x20 mm balls (ZrO2) |
|
|
57 g | |
|
100% < 100 µm | |
|
+ 15ml water | |
|
15 min*1 | |
|
99,9% < 30 µm*2 | |
|
First, we dry grinded the sample for 5min, till it started sticking(see 1a). Then we put 15ml water in the bowl and grinded another 10min. |
|
Download: | 090090_Glas_P6_ZrO2_15min_01.pdf |