500 ml grinding bowl made of zirconium oxide (ZrO2)
+ 800g of 5 mm Ø ZrO2 grinding balls.
Feed quantity:
150 g
Feed Size:
< 100 µm
Additive:
+ 170 ml water
Grinding time:
20 min
Final fineness:
d90 < 3,9 µm 99,2% < 10 µm
Comments:
After a direct grinding time of 10 minutes, bowl temperature rose to > 80 °C
To avoid over pressure, we recommend grinding in steps of 5 minutes, followed by a programmed pausing time of 10 minutes. After several cycles, the outside temperature of the bowl should be checked (remain below 80 °C); grinding time or programmed pausing time might be readjusted afterwards.
After 20 minutes of grinding, desired fineness of d50 < 5 µm has been reached. For a better fineness, still longer grinding times are possible.