M002236 | |
Pharmaceuticals | |
< 300µm | |
d50 < 10µm | |
~ 200 g | |
Higher amount can be ground to d50 < 10µm with our Planetary Mill PULVERISETTE 5 classic line . |
Planetary Mill PULVERISETTE 5 classic line with 4 grinding bowl fastenersmain disk speed: 400 rpm |
||
Equipment: |
500 ml grinding bowl made of agate + 25x 20 mm agate grinding balls |
|
|
200 g | |
|
<300 µm | |
|
4 min | |
|
d90 < 63 µm d50 < 15,5 µm |
|
|
After 4 minutes of dry grinding, sample does not stick to bowl or balls. A longer dry grinding time is still possible (see following result). After 4 minutes of grinding, a fineness of d50 < 16 µm has been detected with our Laser Particle Sizer ANALYSETTE 22. |
Planetary Mill PULVERISETTE 5 classic line with 4 grinding bowl fastenersmain disk speed: 400 rpm |
||
Equipment: |
500 ml grinding bowl made of agate + 25x 20 mm Ø agate grinding balls |
|
|
200 g | |
|
d50 < 15,5 µm (see result 1) | |
|
+ 2 min (∑: 6 min) | |
|
d90 < 59 µm d50 < 12,3 µm |
|
|
After a total of 6 minutes of dry grinding, sample does not stick to bowl or balls. A longer dry grinding time is still possible (see following result). After 6 minutes of grinding, a fineness of d50 < 13 µm has been detected with our Laser Particle Sizer ANALYSETTE 22.
A small portion of sample has been packed for demonstration. |
Planetary Mill PULVERISETTE 5 classic line with 4 grinding bowl fastenersmain disk speed: 400 rpm |
||
Equipment: |
500 ml grinding bowl made of agate + 25x 20 mm Ø agate grinding balls |
|
|
180 g | |
|
d50 < 12,3 µm (see result 2) | |
|
+ 2 min (∑: 8 min) | |
|
d90 < 45,7 µm d50 < 9,8 µm |
|
|
After a total of 8 minutes of dry grinding, sample does not stick to bowl or balls. A longer dry grinding time is still possible (see following result). After 8 minutes of grinding, a fineness of d50 < 10 µm has been detected with our Laser Particle Sizer ANALYSETTE 22.
Even longer grinding times are plausible to reduce the particle size. |
Planetary Mill PULVERISETTE 5 classic line with 4 grinding bowl fastenersmain disk speed: 400 rpm |
||
Equipment: |
500 ml grinding bowl made of agate + 25x 20 mm Ø agate grinidng balls |
|
|
180 g | |
|
d50 < 9,8 µm (see result 3) | |
|
+ 2 min (∑: 10 min) | |
|
d90 < 36,2 µm d50 < 8,7 µm |
|
|
After a total dry grinding time of 10 minutes, sample starts sticking lightly to bowl and balls. For a further reduction of particle size, we recommend grinding in suspension.
The present d50 < 8,7 µm has been detected with our Laser Particle Sizer ANALYSETTE 22. |