M090194 | |
Chemistry | |
100µm | |
d50 5,5µm |
Planetary Micro Mill PULVERISETTE 7 premium line1000 rpm |
||
Equipment: |
80 ml zirconium oxide (ZrO2) bowl with 100g of 2 mm ZrO2 balls. |
|
|
20 g | |
|
100 µm | |
|
+ Toluene (15-18ml)*1 | |
|
4 h | |
|
d50 < 5,7 µm*1 d90 < 10,9 µm |
|
|
*1: each 30min of grinding, we added further 10ml of Toluene.
*2: see our particle size analysis after 4h with ANALYSETTE 22 NanoTec,on Meas.No 7429.
After 30min of grinding, d50 < 9,6µm and d90 < 17,6µm -Meas.No. 7396
Also find the particle size analysis of the original sample (d50 <41,3µm and d90 <73,0µm) on Meas.No. 7390 as well. |
|
Download: | 090194_CuCl_orignal.pdf | |
090194_CuCl_P7pl_2mm_30min.pdf | ||
090194_CuCl_P7pl_2mm_4h.pdf |
Planetary Micro Mill PULVERISETTE 7 premium line1000 rpm |
||
Equipment: |
80 ml zirconium oxide (ZrO2) bowl with 100g of 5 mm ZrO2 balls. |
|
|
20 g | |
|
100 µm | |
|
+ Toluene (15-18ml) | |
|
4 h | |
|
d50 < 7,8 µm*1 d90 < 16,2 µm |
|
|
*1: each 30min of grinding, we added further 10ml of Toluene.
*2: see our partice size analysis after 4h with ANALYSETTE 22 NanoTec,on Meas.No 7428.
After 30min of grinding, d50 < 10µm and d90 < 19,1µm -Meas.No. 7397
|
|
Download: | 090194_CuCl_P7pl_5mm_30min.pdf | |
090194_CuCl_P7pl_5mm_4h.pdf |
Planetary Micro Mill PULVERISETTE 7 premium line850 rpm |
||
Equipment: |
80 ml zirconium oxide (ZrO2) bowl with 25x 10 mm ZrO2 balls. |
|
|
20 g | |
|
100 µm | |
|
+ Toluene (15-18ml)*1 | |
|
1 h | |
|
d50 < 5,5 µm*1 d90 < 11,1 µm |
|
|
*1: each 30min of grinding, we added further 10ml of Toluene.
*2: see our partice size analysis after 1h with ANALYSETTE 22 NanoTec,on Meas.No 7434.
After 30min of grinding, d50 < 6,1µm and d90 < 11,9µm -Meas.No. 7432 It is not possible to grind your sample of Copper chloride (CuCl) within a few hours by using A PULVERISETTE 7 premium line with zirconium oxide grinding set to achieve a fineness < 1µm. |
|
Download: | 090194_CuCl_P7pl_10mm_30min.pdf | |
090194_CuCl_P7pl_10mm_1h.pdf |